Abstract
This investigation was made to develop a method of preparing high - purity
thorium metal in quantities up to 20 kilograms per batch . Several methods for
the preparation , purification , and reduction of thorium tetrachloride are discussed
. Thorium tetrachloride was prepared by chlorination of decomposed
thorium nitrate or oxalate with carbon tetrachloride or phosgene .
tion of the crude tetrachloride was achieved by multiple distillations or by
filtration of the molten chloride . It was found that high - purity thorium metal
could be prepared by sodium reduction of thorium tetrachloride if chloride of
sufficient purity were available . Byproduct salts and excess reductant were
removed by vacuum distillation , and the resultant thorium metal sponge was
consolidated by consumable - electrode or fixed - electrode arc melting . It was
demonstrated that metal prepared by this method could be fabricated into bar ,
rod , or sheet , at room temperature .